Develop kaolin:bentonite mix to replicate #6 Tile kaolin

Share from Insight-live.com (Lab Documentation and Calculation System) by Digitalfire. https://digitalfire.com


Tile #6 Kaolin:Nepheline 70:30

Code #

L3883

Materials Amt
Tile #6 Kaolin 70.000
Nepheline Syenite 30.000

Total:100.00

Notes

This was a series to discover if other kaolins available to us could be augmented with bentonite to approach the working and firing properties of this one.

#6 Tile kaolin is exceptionally plastic on its own, far more so than any other on the market (except Sapphire kaolin). Bentonite is added during production.

Pictures

Tile 6:NS vs. others (with glaze at cone 6)

Left to right: NZK, Grolleg, EPK, Tile 6, Pioneer, McName
The glaze is G2926B transparent.

L3883 Tile #6 Kaolin:Nepheline 70:30 Mix fired bars

Fired cone 3 to 8 (bottom to top).

Kaolins:NS + 2.5% bentonite - cups

McNamee, PIoneer, EPK, Grolleg, NZ.
In all cases, 2.5% bentonite is not enough to produce sufficient plasticity.

Testdata

SHAB - Shrinkage/Absorption

DLEN FLEN FWT BWT CONE DSHR FSHR ABS
894.8585.4834.634.667.85.2%9.9%0.2%
794.6985.6536.5836.86.85.3%9.5%0.6%
594.5384.5335.8836.735.05.5%10.6%2.4%
694.5184.5235.1836.044.85.5%10.6%2.4%
494.4485.8838.8739.854.05.6%9.1%2.5%

LDW - LOI/Density/Water Content

WWGT DWGT FWGT H2O LOI DENS
128.4221.8519.823.1%9.4%

XML (to paste into Insight)

<?xml version="1.0"?> <recipes version="1.0" encoding="UTF-8"> <recipe name="Tile #6 Kaolin:Nepheline 70:30" id="91859" key="tnbv5KG9" date="2026-11-23" codenum="L3883"> <recipelines> <recipeline material="Tile #6 Kaolin" amount="70.000"/> <recipeline material="Nepheline Syenite" amount="30.000"/> </recipelines> </recipe> </recipes>

Born: 2016-08-03, Modified: 2026-11-23 19:06:48

McMamee Kaolin, Nepheline 70:30

Code #

L3896

Materials Amt
*McNamee Clay 70.000
Nepheline Syenite 30.000

Total:100.00

Notes

More plastic than Grolleg or NZK (bout the same as Pioneer kaolin). Same raw appearance and feel also.

With 5% bentonite, plasticity better than 6Tile (at the expense of darker fired color).

SHAB specimen 1: 2.5% bentonite
Specimen 2: 5% bentonite

Pictures

McNamee:Nepheline plus bentonite fired bars cone 6

Top bar: No bentonite.
Middle bar: 2.5% bentonite.
Bottom bar: 5% bentonite.
It is not just the iron in the bentonite that darkens the color. Is also acts as a flux, maturing the body and emphasizing whatever iron is there.

McName:NS vs Tile 6:NS (with glaze at cone 6)

Glaze is G2926B transparent

L3896 - McNamee/NS + 5% Bentonite - cup

Fired at cone 6 with G2926B glaze

Kaolin:NS:5% bentonite kaolin cups fired cone 6

McNamee, PIoneer, EPK, Grolleg, NZ
Each kaolin has 30% nepheline and 5% bentonite (to 70% kaolin).

Notice the crazing on all of them. This is because of a complete lack of silica in the recipe.

Kaolins:NS + 2.5% bentonite - cups

McNamee, PIoneer, EPK, Grolleg, NZ.
In all cases, 2.5% bentonite is not enough to produce sufficient plasticity.

McName Kaolin:Nepheline fired bars

Cone 3 to 8 (bottom to top). No bentonite added.

Testdata

SHAB - Shrinkage/Absorption

DLEN FLEN FWT BWT CONE DSHR FSHR ABS
895.8484.7832.7533.147.84.2%11.5%1.2%
795.8485.1233.8234.386.84.2%11.2%1.7%
695.6985.7833.1433.975.94.3%10.4%2.5%
595.5485.833.9935.194.84.5%10.2%3.5%
495.6985.8634.3835.744.04.3%10.3%4.0%
395.4385.932.7534.673.04.6%10.0%5.9%

LDW - LOI/Density/Water Content

WWGT DWGT FWGT H2O LOI DENS
124.4818.3516.6225.0%9.4%

XML (to paste into Insight)

<?xml version="1.0"?> <recipes version="1.0" encoding="UTF-8"> <recipe name="McMamee Kaolin, Nepheline 70:30" id="92460" key="dPuDxE1J" date="2026-11-23" codenum="L3896"> <recipelines> <recipeline material="McNamee Clay" amount="70.000"/> <recipeline material="Nepheline Syenite" amount="30.000"/> </recipelines> </recipe> </recipes>

Born: 2016-08-16, Modified: 2026-11-23 19:06:54

Pioneer Kaolin:Nepheline 70:30

Code #

L3889

Materials Amt
Pioneer Kaolin 70.000
Nepheline Syenite 30.000

Total:100.00

Notes

This 70:30 mix is part of a test to compare six different kaolins.

The 70:30 mix throws on the potter's wheel with difficulty. While it will lift, walls cannot be thinned to any degree and considerable care must be taken not to develop splits when stretching it.

The 70:30:5 mix (with 5% bentonite), has plasticity that is as good as #6 tile kaolin (without bentonite added). This is the best of the bentonites tested, producing a 70:30 mix that works and fires most similar to #6 Tile.

Pictures

Pioneer:Nepheline plus bentonite fired bars cone 6

Pioneer:NS vs Tile 6:NS (with glaze at cone 6)

These are 70:30 Pioneer:Nepheline fired to cone 6 with G2926B glaze.

Pioneer is whiter with no bentonite additions.

L3889 - Pioneer Kaolin/NS + 5% Bentonite - cup

Kaolins:NS + 2.5% bentonite - cups

McNamee, PIoneer, EPK, Grolleg, NZ.
In all cases, 2.5% bentonite is not enough to produce sufficient plasticity.

Kaolin:NS:5% bentonite kaolin cups fired cone 6

McNamee, PIoneer, EPK, Grolleg, NZ
Each kaolin has 30% nepheline and 5% bentonite (to 70% kaolin).

Notice the crazing on all of them. This is because of a complete lack of silica in the recipe.

Pioneer Kaolin with Nepheline fired bars

Testdata

SHAB - Shrinkage/Absorption

DLEN FLEN FWT BWT CONE DSHR FSHR ABS
896.3786.7237.337.797.83.6%10.0%1.3%
796.286.7238.1638.636.83.8%9.9%1.2%
696.2286.9539.1940.15.93.8%9.6%2.3%
596.1887.1940.1741.464.83.8%9.3%3.2%
496.1187.1640.0741.724.03.9%9.3%4.1%
396.2587.9238.7640.853.03.8%8.7%5.4%

DFAC - Drying Factor

DFAC SOLD
1A000nil

LDW - LOI/Density/Water Content

WWGT DWGT FWGT H2O LOI DENS
126.3120.6318.6921.6%9.4%

XML (to paste into Insight)

<?xml version="1.0"?> <recipes version="1.0" encoding="UTF-8"> <recipe name="Pioneer Kaolin:Nepheline 70:30" id="92290" key="q2eMQN7Z" date="2026-11-23" codenum="L3889"> <recipelines> <recipeline material="Pioneer Kaolin" amount="70.000" tolerance=""/> <recipeline material="Nepheline Syenite" amount="30.000" tolerance=""/> </recipelines> </recipe> </recipes>

Born: 2016-08-03, Modified: 2026-11-23 19:07:00

EP Kaolin, Nepheline 70:30

Code #

L3890

Materials Amt
EPK 70.000
Nepheline Syenite 30.000

Total:100.00

Notes

This material does not throw well at all as a pure material, not even close to #6 tile. It feels like swamp mud!

Throwing of the material having 5% added bentonite was good. 2.5% tore badly when cut (although throwable).

SHAB specimen 1: 2.5% bentonite
Specimen 2: 5% bentonite

Pictures

EPK:Nepheline with bentonite additions bars cone 6

Top bar: No bentonite added.
Middle bar: 2.5% bentonite.
Bottom bar: 5% bentonite.

EPK:NS vs Tile 6:NS (with glaze at cone 6)

Glaze is G2926B transparent

L3890 - EPK/NS + 5% Bentonite - cup

Fired at cone 6 with G2926B glaze

Goopy plastic consistency

The material was plastic one day and then turned to this two days later.

Kaolins:NS + 2.5% bentonite - cups

McNamee, PIoneer, EPK, Grolleg, NZ.
In all cases, 2.5% bentonite is not enough to produce sufficient plasticity.

Kaolin:NS:5% bentonite kaolin cups fired cone 6

McNamee, PIoneer, EPK, Grolleg, NZ
Each kaolin has 30% nepheline and 5% bentonite (to 70% kaolin).

Notice the crazing on all of them. This is because of a complete lack of silica in the recipe.

EPK with Nepheline fired bars

Cone 3 to 8 (bottom to top). No bentonite added.

Testdata

SHAB - Shrinkage/Absorption

DLEN FLEN FWT BWT CONE DSHR FSHR ABS
894.5182.933.8634.017.85.5%12.3%0.4%
794.4683.235.0135.166.85.5%11.9%0.4%
694.2282.8435.1135.275.95.8%12.1%0.5%
594.0482.7836.2136.394.86.0%12.0%0.5%
494.1382.9537.8138.154.05.9%11.9%0.9%
394.1183.1535.9336.493.05.9%11.6%1.6%

LDW - LOI/Density/Water Content

WWGT DWGT FWGT H2O LOI DENS
125.2719.317.4223.6%9.7%
210.987.729.9%
317.2813.4622.1%

XML (to paste into Insight)

<?xml version="1.0"?> <recipes version="1.0" encoding="UTF-8"> <recipe name="EP Kaolin, Nepheline 70:30" id="92291" key="emFBjGNn" date="2026-11-23" codenum="L3890"> <recipelines> <recipeline material="EPK" amount="70.000" tolerance=""/> <recipeline material="Nepheline Syenite" amount="30.000" tolerance=""/> </recipelines> </recipe> </recipes>

Born: 2016-08-03, Modified: 2026-11-23 19:07:06

Grolleg Kaolin, Nepheline 70:30

Code #

L3892

Materials Amt
NZ Kaolin 70.000
Nepheline Syenite 30.000

Total:100.00

Notes

Of the kaolins compared, this is the most fragile in the dry state. Also the least plastic, despite the fact that it is the stickiest of all of them (the NZK a close second). Grolleg does respond fairly well to added bentonite. At 3.3% bentonite, this is plastic enough to make the same size vessel as 6Tile, but not nearly as easily (it is more wobbly). At 5% bentonite, it is better, but still not as good as 6Tile (whereas the fired color, with bentonite, is considerably darker than #6 tile).

This reaches zero porosity by cone 5 so it obviously contains impurities that, although low in iron oxide, help to mature it. UK kaolins are known for needing less feldspar when used in a porcelain recipe.

Pictures

Grolleg:Nepheline with bentonite additions fire bars cone 6

Top bar: No bentonite.
Middle bar: 2.5% bentonite.
Bottom bar: 5% bentonite.
The bentonite is acting as a flux, maturing the body to look more like a porcelain.

NZK:NS vs Tile 6:NS (with glaze at cone 6)

Glaze is G2926B transparent

L3892 - NZK/NS + 5% Bentonite - cup

Fired at cone 6 with G2926B glaze

Kaolin:NS:5% bentonite kaolin cups fired cone 6

McNamee, PIoneer, EPK, Grolleg, NZ
Each kaolin has 30% nepheline and 5% bentonite (to 70% kaolin).

Notice the crazing on all of them. This is because of a complete lack of silica in the recipe.

Grolleg Kaolin with Nepheline fired bars

Cone 3 to 8 (bottom to top). No bentonite added.

Testdata

SHAB - Shrinkage/Absorption

DLEN FLEN FWT BWT CONE DSHR FSHR ABS
895.8185.2737.0937.17.84.2%11.0%0.0%
795.7585.1237.8137.826.84.3%11.1%0.0%
696.0185.537.8137.825.94.0%10.9%0.0%
596.2385.8535.5135.524.83.8%10.8%0.0%
496.2386.235.2435.274.03.8%10.4%0.1%
396.2987.134.5535.763.03.7%9.5%3.5%

LDW - LOI/Density/Water Content

WWGT DWGT FWGT H2O LOI DENS
125.6319.4917.8624.0%8.4%

XML (to paste into Insight)

<?xml version="1.0"?> <recipes version="1.0" encoding="UTF-8"> <recipe name="Grolleg Kaolin, Nepheline 70:30" id="92293" key="euqWoeqW" date="2026-11-23" codenum="L3892"> <recipelines> <recipeline material="NZ Kaolin" amount="70.000" tolerance=""/> <recipeline material="Nepheline Syenite" amount="30.000" tolerance=""/> </recipelines> </recipe> </recipes>

Born: 2016-08-03, Modified: 2026-11-23 19:07:14

NZ Kaolin:Nepheline 70:30

Code #

L3891

Materials Amt
Grolleg Kaolin 70.000
Nepheline Syenite 30.000

Total:100.00

Notes

Unbelievably sticky. Even with 5% bentonite, while I can pull a mug up to height, it is not even close to 6Tile kaolin in plasticity.
The glaze is G2926B transparent.

Bars are mislabelled at L3892
L3842 Tile6

Pictures

New Zealand Kaolin plus bentonite cone 6 fired bars

Grolleg:NS vs Tile 6:NS (with glaze at cone 6)

Glaze is G2926B transparent.

L3891 - Grolleg/NS + 5% Bentonite - cup

Kaolins:NS + 2.5% bentonite - cups

McNamee, PIoneer, EPK, Grolleg, NZ.
In all cases, 2.5% bentonite is not enough to produce sufficient plasticity.

Kaolin:NS:5% bentonite kaolin cups fired cone 6

McNamee, PIoneer, EPK, Grolleg, NZ
Each kaolin has 30% nepheline and 5% bentonite (to 70% kaolin).

Notice the crazing on all of them. This is because of a complete lack of silica in the recipe.

New Zealand kaolin with Nepheline fired bars

Testdata

SHAB - Shrinkage/Absorption

DLEN FLEN FWT BWT CONE DSHR FSHR ABS
195.3485.733.9333.937.84.7%10.1%0.0%
293.5784.2934.2134.217.86.4%9.9%0.0%
895.7679.6632.232.227.84.2%16.8%0.1%
795.1679.6432.7232.776.84.8%16.3%0.2%
694.7179.4532.0932.125.95.3%16.1%0.1%
595.279.9731.8332.214.84.8%16.0%1.2%
495.7781.1330.9131.614.04.2%15.3%2.3%
395.8682.0129.0630.243.04.1%14.4%4.1%

LDW - LOI/Density/Water Content

WWGT DWGT FWGT H2O LOI DENS
124.5118.0416.2526.4%9.9%

XML (to paste into Insight)

<?xml version="1.0"?> <recipes version="1.0" encoding="UTF-8"> <recipe name="NZ Kaolin:Nepheline 70:30" id="92292" key="WfPnHcnZ" date="2026-11-23" codenum="L3891"> <recipelines> <recipeline material="Grolleg Kaolin" amount="70.000" tolerance=""/> <recipeline material="Nepheline Syenite" amount="30.000" tolerance=""/> </recipelines> </recipe> </recipes>

Born: 2016-08-03, Modified: 2026-11-23 19:07:23